Custom Deep Drawing Services

Deep drawn sheet metal components — cups, covers, housings, caps and shallow enclosures — produced from customer drawings in SPCC, 304 stainless, aluminium and copper, on 30–400T presses with controlled blank-holding force.

Deep drawing is the process where the metal flows rather than folds. That distinction matters: a drawn part has a wall thickness that changed during forming, and a drawing that ignores it will fail at the third stage rather than the first.

What we deep draw

Draw ratio: how many stages a part needs

The draw ratio is the blank diameter divided by the punch diameter. Each material tolerates a maximum ratio per stage; exceed it and the wall tears near the punch radius.

As a working guide, the first draw in mild steel typically removes up to about half the blank diameter, and each subsequent stage removes less. Stainless tolerates less per stage because it work hardens, so a cup that draws in two stages in SPCC may need three or four in 304.

What this means practically: a deeper part is not harder because it is deep, it is harder because it needs more stages. Each stage is a die station, a handling step and a chance for wall thinning. We confirm the stage count and the achievable depth during drawing review, before tooling.

Thickness range and an honest limit

Our presses handle 0.5–10 mm material, but deep drawing and heavy plate are not the same job. Our deep drawing work sits mostly in the 0.5–4 mm band. Above that, drawing force and blank-holding requirements climb steeply, and for many geometries a welded or bent-and-formed assembly is the more sensible route than a very large draw.

If your part is thick and deep, we will say so at enquiry and suggest an alternative process rather than quote a draw we cannot hold.

Materials for drawing

Material Drawing behaviour Practical note
SPCC cold-rolled steel Good — the standard choice Consistent thickness gives predictable wall thinning
Q235 carbon steel Good at moderate depth Softer, less springback than stainless; watch surface finish
304 stainless Work hardens quickly Needs more stages and inter-stage annealing at higher reductions
Aluminium Forms easily, tears if pushed Annealed temper draws far better; galling risk on the die
Copper, brass Excellent drawability Good for deep electrical and decorative draws; galling needs die attention

Material and finish detail: materials and surface finishing.

The four failure modes and what causes them

  1. Wrinkling at the flange. Insufficient blank-holding force, or a blank that is too large for the first stage. Corrected by blank-holder pressure and blank size, not by a larger press.
  2. Tearing at the punch radius. Too much reduction in one stage. The fix is an extra stage, a larger punch radius, or a more drawable material temper.
  3. Wall thinning and a raised rim. Normal in drawing, but it must be anticipated. If the drawing calls a uniform wall thickness, it cannot be met — the wall thins as material flows from the flange.
  4. Earing. Anisotropy in rolled sheet produces a wavy rim. Usually trimmed in a later operation; if the rim is visible, plan for trimming.

Knowing which of these applies to your geometry is what a drawing review is for. It is also why we do not quote a deep drawn part from an outline alone.

Drawing plus secondary operations

Most drawn parts need more than the draw. Pierced holes, trimmed rims, flanged edges, embossed features and threaded inserts are usually added in the same tool or in a following station. Building them into the die from the start is cheaper than adding a second tool later.

Finishing applies after forming: zinc plating, powder coating, electrophoresis and deburring, selected by corrosion and appearance requirement. Electrophoresis is often the practical choice for drawn enclosures because it reaches inside the drawn section.

Specification summary

Materials SPCC, Q235, 304 stainless, copper, brass, aluminium
Thickness 0.5–10 mm for stamping; deep drawing practical range 0.5–4 mm
Press range 30–400 T
Stages Single and multi-stage draws, confirmed per geometry
Secondary operations Piercing, trimming, flanging, embossing in the same or following station
Finishing Zinc plating, powder coating, electrophoresis, deburring
Sampling 7 days after requirements are confirmed
Production 15–25 days after sample approval
Inspection Height gauges, fixtures, CMM; wall thickness checks

Frequently asked questions

How deep can you draw in one stage?

It depends on material, thickness and diameter. Mild steel tolerates roughly half the blank diameter in the first stage; stainless considerably less. We confirm the stage count for your geometry during review.

Can the wall thickness stay the same as the blank?

No. Material flows from the flange into the wall, so the wall thins and the rim thickens slightly. If your drawing specifies uniform thickness, it needs revising — this is one of the most common drawing corrections we raise.

Do you anneal between stages?

For stainless and heavily reduced draws, yes — inter-stage annealing restores ductility. It adds a step and is priced accordingly, which is why the stage count matters to the quotation.

Can you draw a rectangular box?

Yes, within limits. Rectangular draws are less uniform than round ones: the corners need more stages than the sides, and the blank shape is not a simple circle. Send the geometry and we will confirm feasibility.

Can drawn parts be plated after forming?

Yes. Electrophoresis is often the better option for enclosures because it coats the inside of the drawn section. Zinc plating works for simpler geometries.

Request a quote

Send the drawing, material and temper, thickness, quantity and target date to robert@hmstamping.com, or use the quote request form. For drawn parts, include the internal depth and any wall-thickness requirement — those two figures decide the stage count.

Related: metal stamping · sheet metal bending · custom metal stamping parts · prototype process comparison

◌

LET’S TALK ABOUT YOUR PART

Request a quote

Share your drawing, material and quantity.

Request for quotation

    By submitting this form you agree to be contacted about your enquiry.

    Custom stamping parts made to drawingRequest a quoteWhatsApp
    Export support for customers in Malaysia, Vietnam and Thailand · See what to send for a quote